Loss of resilience
The seal still fills the groove but no longer pushes back hard enough. A small movement in the hardware or a pressure change is enough to open a leak path.
Elastomer seals and O-rings that stay flexible and keep sealing when the temperature falls, from arctic wellheads and gas blow-down to cold-climate hydraulics.
Most elastomers stiffen and lose their sealing force long before they freeze solid. ISMAT's low-temperature range covers nine grades across four polymer families, each compounded to stay elastic in the cold without giving up the fluid resistance or strength the job needs.
An elastomer seals because it is elastic. Squeezed into a groove, it pushes back against the metal faces and keeps pushing as pressure and temperature change. Cold takes that ability away gradually: the polymer chains move closer together and lose their freedom to move, the rubber turns leathery, then stiff and at its glass transition temperature (Tg) it behaves like hard plastic.
The seal still fills the groove but no longer pushes back hard enough. A small movement in the hardware or a pressure change is enough to open a leak path.
Elastomers shrink more than ten times as much as steel for every degree of cooling. Squeeze falls just as the material becomes least able to make up for it.
A stiff seal cannot follow a valve stem, a shaft or a pressure reversal. Leaks often show at start-up or on the first actuation after a cold soak.
A seal held compressed in the cold can take a set and leak once it warms up. Below its brittle point, a sudden impact can crack it.
Oil and gas equipment in Canada, Alaska, Russia and northern Europe runs all year where winter temperatures reach -40°C or lower. High-altitude aircraft systems face similar conditions.
When high-pressure gas is vented quickly, during a blow-down for example, the expanding gas cools sharply and can chill valves and seals far below the ambient temperature.
Cold stiffening is a physical change, not a chemical one. A seal taken below its limit will normally recover as it warms, provided it was not disturbed or shock-loaded while it was brittle.
Each bar shows the operating range from the grade's technical data sheet, on one scale from -60°C to +240°C. Filter by the lowest temperature your equipment will see and by what else the seal has to cope with. Select a grade to open its data sheet page.
Showing all 9 grades
Rapid gas decompression: certified to NORSOK M-710. Sour gas: Vertex FC 15 is certified to NACE TM0187 and API 6A; the Vertex F grades show under 10% volume swell in sour gas on ISMAT's data sheets. All nine grades resist mineral oils and hydrocarbons.
FKM is one of the most widely used high-performance seal materials, but conventional grades typically lose their flexibility somewhere between -15°C and -25°C. ISMAT's low-temperature FKM grades use terpolymer chemistry developed for cold flexibility, so the seal keeps the fuel, oil and chemical resistance that FKM is chosen for at temperatures that would leave a standard grade rigid.
Vertex FC 24ULT is rated from -60°C to +204°C, the lowest limit of any grade on this page, with a compression set of 20% maximum after 22 hours at 200°C. Vertex FC 15 combines a -46°C rating with certification for rapid gas decompression, sour fluid immersion and CO2 decompression, which suits it to cold gas service in oil and gas. Vertex FC 15A is a softer 75 Shore A version with 150% minimum elongation, for seals that need easier fitting or lower sealing force.
Available as
| Trade name | Hardness | Min. temp | Max. temp | Key data and certifications |
|---|---|---|---|---|
| Vertex FC 24ULT | 90±5 | -60°C | +204°C |
|
| Vertex FC 15 | 90±5 | -46°C | +204°C |
|
| Vertex FC 15A | 75±5 | -46°C | +204°C |
|
Nitrile is the usual choice for oil and fuel service and normally the most economical one. Its low-temperature behaviour depends heavily on the compound, and the trade-off is real: nitrile grades built for the cold tend to swell more in some oils and fuels. The balance between flexibility and fluid resistance has to be set for the job.
Cerulean N 02LT and Cerulean N 04LT are both rated from -55°C to +107°C. N 02LT is an 80 Shore A copolymer NBR with strong resistance to oils and hydrocarbon solvents, used in hoses, pumps, oil seals and cable sealing. N 04LT is a softer 70 Shore A grade with good mechanical strength and abrasion resistance, for valves, pumps, mechanical seals and compressors.
Available as
| Trade name | Hardness | Min. temp | Max. temp | Key data |
|---|---|---|---|---|
| Cerulean N 02LT | 80±5 | -55°C | +107°C |
|
| Cerulean N 04LT | 70±5 | -55°C | +107°C |
|
HNBR is nitrile whose polymer backbone has been saturated by hydrogenation. It keeps the oil resistance of NBR and adds higher mechanical strength, better heat resistance and much better resistance to ozone and weathering, which matters for equipment that stands outdoors through the winter.
Both Vertex H grades are rated from -46°C, with short-term exposure to -52°C. Vertex H 17 is certified to NORSOK M-710 for rapid gas decompression and to NACE TM0192 for CO2 decompression. Its typical results include a tensile strength of 19 MPa, a compression set of 5.4% after 22 hours at 150°C and a TR10 of -37°C. Vertex H 18LT is an 85 Shore A grade rated to +150°C, for valves, pumps, mechanical seals and compressors.
Available as
| Trade name | Hardness | Min. temp | Max. temp | Key data and certifications |
|---|---|---|---|---|
| Vertex H 17 | 87 (typical) | -46°C -52°C short-term |
+160°C |
|
| Vertex H 18LT | 85±5 | -46°C -52°C short-term |
+150°C |
|
FFKM is fully fluorinated, which gives it the widest chemical resistance of any elastomer. Most FFKM grades are designed for heat rather than cold. ISMAT's standard Vertex F grades, such as Vertex F 02, are rated to -10°C.
Vertex F 02LT and Vertex F 07LT extend that limit to -40°C. They resist hot organic and inorganic acids, caustics, amines, ketones, aldehydes, esters, ethers, alcohols, fuels, solvents, sour gases, hydrocarbons, steam, hot water, ethylene and propylene oxide and mixed process streams. F 02LT (75 Shore A) is rated to +230°C; F 07LT (90 Shore A) is rated to +240°C, and its higher hardness helps where extrusion resistance matters.
Volume swell, Vertex F 02LT and F 07LT
Source: ISMAT technical data sheets, Vertex F 02LT and F 07LT.
Available as
| Trade name | Hardness | Min. temp | Max. temp | Key data |
|---|---|---|---|---|
| Vertex F 02LT | 75±5 | -40°C | +230°C |
|
| Vertex F 07LT | 90±5 | -40°C | +240°C |
|
Limits: do not use any Vertex F grade with molten alkali metals. Hot amines above +70°C cause 10-30% swell and fluorinated fluids 30-50%, so check these media with ISMAT before specifying.
Specification values from ISMAT's technical data sheets. Values marked * are typical test results; all others are specification limits.
Swipe the table sideways to see every column →
| Grade | Hardness, Shore A | Density, g/cc | Tensile, MPa | Elongation, % | Compression set | Operating range | Certifications |
|---|---|---|---|---|---|---|---|
| Terpolymer FKM - Vertex FC | |||||||
| Vertex FC 24ULT | 90±5 | 1.85±0.05 | 14 min | 80 min | 20% max (22 h/200°C) 35% max (70 h/200°C) | -60°C to +204°C | - |
| Vertex FC 15 | 90±5 | 1.85±0.05 | 10 min | 80 min | 25% max (22 h/200°C) 35% max (70 h/200°C) | -46°C to +204°C | NORSOK M-710, API 6A, NACE TM0187, NACE TM0192 |
| Vertex FC 15A | 75±5 | 1.85±0.05 | 10 min | 150 min | 30% max (70 h/200°C) | -46°C to +204°C | - |
| NBR - Cerulean N (N 02LT is a copolymer NBR) | |||||||
| Cerulean N 02LT | 80±5 | - | 7 min | 120 min | 30% max (22 h/100°C) 50% max (70 h/100°C) | -55°C to +107°C | - |
| Cerulean N 04LT | 70±5 | - | 8 min | 150 min | 30% max (22 h/100°C) 50% max (70 h/100°C) | -55°C to +107°C | - |
| Hydrogenated nitrile (HNBR) - Vertex H | |||||||
| Vertex H 17 | 87* | 1.304* | 19.02* | 143.44* | 5.36%* (22 h/150°C) 11.86%* (70 h/150°C) | -46°C to +160°C -52°C short-term | NORSOK M-710, NACE TM0192 |
| Vertex H 18LT | 85±5 | 1.30±0.05 | 14 min | 100 min | 25% max (22 h/150°C) | -46°C to +150°C -52°C short-term | - |
| Perfluoroelastomer (FFKM) - Vertex F | |||||||
| Vertex F 02LT | 75±5 | 1.95±0.05 | 10 min | 120 min | 30% max (24 h/200°C) | -40°C to +230°C | - |
| Vertex F 07LT | 90±5 | 2.0±0.05 | 11.3 min | 80 min | 30% max (24 h/200°C) | -40°C to +240°C | - |
Test methods: hardness ASTM D2240; density ASTM D792; tensile strength and elongation ASTM D412; compression set ASTM D395 Method B; TR10 ASTM D1329. Full data sheets can be downloaded from each grade page.
A low-temperature figure is only useful if you know how it was measured. Each test describes something different and two tests on the same compound can give answers several degrees apart.
A specimen is stretched, frozen and then warmed slowly. TR10 is the temperature at which it has recovered 10% of the stretch, close to the point where it starts to behave like rubber again. It is the most practical single figure for comparing seal compounds.
The temperature below which the polymer is glass-like. A seal does not work there. TR10 usually sits a few degrees above Tg.
The lowest temperature at which a specimen survives an impact without cracking. It shows the material will not shatter, not that it will still seal.
Measures how stiff the rubber becomes as it cools. The temperature at which the modulus reaches 70 MPa (T70) is often taken as the limit of useful flexibility and usually falls close to TR10.
Measures how well a compressed specimen recovers after cold exposure. Because it reproduces the way a seal is loaded, it is a good guide to real sealing behaviour.
The most reliable check is a seal tested in a housing that reproduces the real groove fill, squeeze, surface finish, pressure and media. Laboratory tests compare compounds; functional tests confirm the design.
A widely used guideline for O-rings and other compression seals: a dynamic seal should not run below its TR10, while a static seal in a well-designed groove typically seals to about 8°C below it.
Example: Vertex H 17 has a measured TR10 of -37°C. Applying the static guideline gives about -45°C, close to its -46°C rated limit. For a dynamic seal, plan on -37°C.
The operating temperatures on this page are taken from each grade's technical data sheet. For dynamic duty near the lower limit or where a rating must be tied to a specific test, ask ISMAT for the test data on the grade you are considering.
The compound is the starting point, not the whole answer. These factors change how low a given material will actually seal in your equipment.
Pressure raises the glass transition temperature, by roughly 1°C for every 52 bar (750 psi). A compound that seals at -40°C at low pressure may not do so at several hundred bar.
Seals pressurised before they cool tend to seal at lower temperatures than seals pressurised when they are already cold and stiff.
A seal loaded from one side moves less in its groove than one that sees pressure reversals, so it holds a seal better in the cold.
More squeeze helps static seals at low temperature, but it must be balanced against fitting damage and against thermal expansion if the system also runs hot. Check groove fill at the lowest temperature, not only at assembly.
A small amount of swell from hydrocarbons softens the seal and raises interference, which helps. Fluids that extract plasticiser do the opposite and leave a harder, smaller seal. Share the full fluid list with us.
Lubrication improves low-temperature sealing, but it can be wiped away in service. Base the design on the unlubricated seal.
Groove geometry and surface finish both affect how a stiffening seal behaves. Where cold and high pressure combine, back-up rings protect the seal from extrusion.
For critical service, test the seal in a fixture that reproduces the real housing, pressure and media before you commit to it.
Below -60°C, and in cryogenic service such as LNG and liquid nitrogen, elastomers are no longer the right material. For these conditions ISMAT uses PTFE and PCTFE grades from the Novum range, including spring-energised seals that supply the sealing force the material cannot.
Cold service rarely comes alone. It arrives with gas pressure, sour fluids, fuels or aggressive chemicals and the grade has to handle all of them together.
Wellhead and valve seals in arctic and winter fields, gas compressors and equipment exposed to blow-down cooling.
ExploreValves, pumps, mechanical seals and reactors handling cold process streams and refrigerated chemicals.
ExploreHydraulic and fuel system seals that must keep working at high-altitude temperatures.
ExploreGas and power infrastructure in cold climates, including compressors and outdoor valve stations.
ExploreFuel, hydraulic and driveline seals for vehicles that start and run through sub-zero winters.
ExploreHydraulics and earth-moving equipment working in cold regions, where abrasion and oil resistance matter too.
ExploreIf your question is not answered here, ISMAT's engineers will help you choose a grade.
Vertex FC 24ULT, a terpolymer FKM, is rated from -60°C to +204°C. The Cerulean N 02LT and N 04LT nitrile grades reach -55°C, the Vertex H 17 and H 18LT HNBR grades -46°C (-52°C short-term) and the Vertex F 02LT and F 07LT perfluoroelastomers -40°C. Below -60°C, ISMAT uses PTFE and PCTFE cryogenic seals instead.
TR10 (ASTM D1329, ISO 2921) is the temperature at which a stretched, frozen rubber specimen has retracted by 10% as it warms. It marks roughly where the compound starts to behave like rubber again, so it is the most practical single figure for comparing seal compounds. As a guide, a dynamic seal should not run below its TR10, while a static seal in a well-designed groove typically seals to about 8°C below it.
Usually, yes. Cold stiffening is a physical change, so a seal normally returns to its original properties when it warms up, provided it was not disturbed or shock-loaded while brittle. The real risks are leakage while the seal is cold and compression set if it was held squeezed in the cold.
Vertex FC 15 (FKM, -46°C) and Vertex H 17 (HNBR, -46°C) are certified to NORSOK M-710 for rapid gas decompression and to NACE TM0192 for CO2 decompression. Vertex FC 15 is also certified to NACE TM0187 (sour fluid immersion, 20% H2S) and to API 6A (10% H2S at 200°C).
NBR is the most economical choice for mineral oils, greases and fuels within -55°C to +107°C. HNBR adds mechanical strength, heat resistance to +150°C or +160°C and much better ozone and weather resistance. FKM is the choice when the fluid or temperature is beyond HNBR, for example aromatic fuels, many chemicals or continuous service up to +204°C. FFKM covers aggressive chemicals that FKM cannot handle.
Yes. Pressure raises the glass transition temperature of an elastomer by roughly 1°C for every 52 bar (750 psi), so high-pressure gas service needs more margin below the rated limit. Applying pressure before the seal cools also tends to improve low-temperature sealing.
Each grade page has a downloadable technical data sheet, and the ISMAT Chemical Compatibility Guide covers media resistance across all materials. For test data beyond the data sheet, such as TR10 or certification reports, contact ISMAT.
How rapid gas decompression damages elastomer seals, and what certified grades are tested for.
Read article Material selectionA side-by-side look at three fluoroelastomer families and where each one fits.
Read article Sour gasWhy sour gas attacks many elastomers and how perfluoroelastomers resist it.
Read articleSend the operating conditions below and ISMAT's engineers will recommend a grade and share the test data behind the recommendation.
The information on this page is accurate and reliable to the best of ISMAT's knowledge, but it does not guarantee the performance of a finished part. Customers should evaluate parts before use, especially in applications where failure could cause injury or damage.